Register of building materials used for this application, cross-section
(from outside to inside)
|
Thickness [mm] |
Building material |
Thermal performance |
Reaction to fireklasse EN |
λ |
μ min – max |
ρ |
c |
A |
10,0
|
plaster
|
1,000
|
10-35
|
2000
|
1,130
|
A1
|
B |
50,0
|
wood wool composite boards
|
0,090
|
2-5
|
370
|
2,000
|
B
|
C |
10,0
|
gypsum fibre board
|
0,320
|
21
|
1000
|
1,100
|
A2
|
D |
|
construction timber
(60/..; e=*)
|
0,120
|
50
|
450
|
1,600
|
D
|
E |
|
- variable insulation material
|
|
|
|
|
|
F |
12,5
|
gypsum fibre board
|
0,320
|
21
|
1000
|
1,100
|
A2
|
G |
|
vapour barrier sd≥ 4m
|
|
|
1000
|
|
|
H |
|
spruce wood
cross battens (a=400) or battens offset)
|
0,120
|
50
|
450
|
1,600
|
D
|
I |
|
- variable insulation material
or air layer in type 02
|
|
|
|
|
|
J |
12,5
|
gypsum plaster board type DF
or
|
0,250
|
10
|
800
|
1,050
|
A2
|
J |
12,5
|
gypsum fibre board
|
0,320
|
21
|
1000
|
1,100
|
A2
|
Variations of building components
|
Thickness of layer |
Note |
Fire performance |
Thermal performance |
Acoustic performance |
Eco Sustainability |
Mass |
|
Thickness [mm] |
Building material |
Σ |
REI |
U [W/(m²K)] |
Diffusion |
Rw (C,Ctr) [dB] |
ΔOI3 |
m [kg/m²] |
awropi10b-00
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
289,0
|
e=625
|
60
from inside
60
from outside
|
0,20
|
adequate
|
52
(-3,-8)
|
28,24
|
69,5
|
awropi10b-01
|
D
E
H
I
|
120,0
120,0
40,0
40,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
249,0
|
e=625
|
60
from inside
60
from outside
|
0,24
|
adequate
|
51
(-3,-8)
|
25,59
|
67,0
|
awropi10b-03
|
D
E
H
I
|
200,0
200,0
40,0
40,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
329,0
|
e=625
|
60
from inside
60
from outside
|
0,17
|
adequate
|
53
(-3,-8)
|
30,88
|
72,0
|
awropi10b-04
|
D
E
H
I
|
240,0
240,0
40,0
40,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
369,0
|
e=625
|
60
from inside
60
from outside
|
0,15
|
adequate
|
54
(-3,-8)
|
33,53
|
74,5
|
awropi10b-05
|
D
E
H
I
|
200,0
200,0
80,0
80,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
369,0
|
e=625
|
60
from inside
60
from outside
|
0,15
|
adequate
|
53
(-3,-8)
|
33,26
|
75,1
|
awropi10b-06
|
D
E
H
I
|
240,0
240,0
80,0
80,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
409,0
|
e=625
|
60
from inside
60
from outside
|
0,13
|
adequate
|
54
(-3,-8)
|
35,91
|
77,5
|
awropi10b-07
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
mineral wool [035; 50; <1000°C]
spruce wood
mineral wool [035; 50; <1000°C]
|
289,0
|
e=625
|
60
from inside
60
from outside
|
0,18
|
adequate
|
53
(-3,-8)
|
50,80
|
75,6
|
awropi10b-08
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
mineral wool [038; ≥33; ≥1000°C]
spruce wood
mineral wool [038; ≥33; ≥1000°C]
|
289,0
|
e=625
|
60
from inside
60
from outside
|
0,20
|
adequate
|
52
(-3,-8)
|
34,06
|
72,5
|
awropi10b-09
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
cellulose fibre [0,040; R=55]
spruce wood
cellulose fibre [0,040; R=55]
|
289,0
|
e=625
|
60
from inside
60
from outside
|
0,20
|
adequate
|
52
(-3,-8)
|
21,37
|
76,5
|
awropi10b-10
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
sheep wool [0,041; R=26]
spruce wood
sheep wool [0,041; R=26]
|
289,0
|
e=625
|
60
from inside
60
from outside
|
0,22
|
adequate
|
52
(-3,-8)
|
22,19
|
69,5
|
awropi10b-11
|
D
E
H
I
|
160,0
160,0
40,0
40,0
|
construction timber
mineral wool [040; ≥16; <1000°C]
spruce wood
mineral wool [040; ≥16; <1000°C]
|
289,0
|
e=400
|
60
from inside
60
from outside
|
0,21
|
adequate
|
52
(-3,-8)
|
27,83
|
73,7
|
Last update 02.08.2023/hfa.eco2soft